Nilo 36• • Trade name of Special Metals Group of Companies
W.NR 1.3912
UNS K93600
UNS K93601
AWS 090
UNS K93600
UNS K93601
AWS 090
A Nickel-Iron, low expansion alloy containing 36% Nickel. It maintains near constant dimensions over the range of normal atmospheric temperatures and has a low coefficient of expansion from cryogenic temperatures to about 500oC (930oF). Nilo 36 also retains good strength and toughness at cryogenic temperatures.
Applications include:
- Standards of Length
- Thermostat Rods
- Laser Components
- Tanks and Piping for the Storage and Transportation
of Liquefied Gasses
| Approximate Chemical Composition | |
| Ni | 35-38% |
| Fe | BAL |
| DENSITY | 8.11 g/cm3 | 0.293 lb/in3 |
| MELTING POINT | 1430oC | 2610oF |
| INFLECTION POINT | 220°C | 430°F |
| THERMAL CONDUCTIVITY | 10.0 W/m•°C | 69.3 btu•in/ft2•h°F |
| COEFFICIENT OF EXPANSION | 1.5 µm/m °C ( 20 - 100°C) 2.6 µm/m °C |
0.83 x 10-6 in/in
°F ( 70 - 212°F) 1.4 x 10-6 in/in
°F |
|
HEAT TREATMENT (AFTER FORMING) |
|
| The Nilo alloys are usually used in the annealed condition (residual cold work distorts the coefficients of thermal expansion) | |
| Anneal at 850 - 1000°C (1560 - 1830°F) | |
| For highest dimensional stability, heat treat as follows: | Anneal at 830°C (1525°F) for 30 minutes and water quench, re-heat to 300°C (570°F) for 1 hour and water quench. Finally re-heat to 100°C (212°F) for 48 hours and air cool. |
| CONDITION |
APPROX TENSILE STRENGTH |
APPROX SERVICE TEMPERATURE |
||||
| Annealed | 450-550 N/mm2 | 65-80 ksi | up to 500oC | up to 930oF | ||
| Hard Drawn | 700-900 N/mm2 | 102-131 ksi | up to 500oC | up to 930oF | ||
| STANDARDS |
| - |